We are manufacturers of outdoor furniture and manufacture HDPE wicker (Plastic Cane) to be used in our furniture. Visit our website www.loomcrafts.com to see our products. We manufacture our wicker using HDPE (Bought from Reliance) and add UV in it. This wicker has to be very durable for outdoor conditions as this furniture is used all the time in outdoors. We are facing a problem of breakage of our wicker after some time of usage. Please suggest us if any kind of additive can be added so as to increase the tensile strength of the cane.
We are manufacturers of outdoor furniture and manufacture HDPE wicker (Plastic Cane) to be used in our furniture. Visit our website www.loomcrafts.com to see our products. We manufacture our wicker using HDPE (Bought from Reliance) and add UV in it. This wicker has to be very durable for outdoor conditions as this furniture is used all the time in outdoors. We are facing a problem of breakage of our wicker after some time of usage. Please suggest us if any kind of additive can be added so as to increase the tensile strength of the cane.





RE: HDPE Wicker
Suppliers of UV stabilizers like Ciba can provide assistance, if they're not already.
Good luck!
Tom Jablonowski, TSE Industries, Inc.
www.tse-industries.com
RE: HDPE Wicker
RE: HDPE Wicker
TTFN
FAQ731-376: Eng-Tips.com Forum Policies
RE: HDPE Wicker
tom
RE: HDPE Wicker
UV protection does is not the same thing from one supplier to another. There are lots of different additives, some better some worse and one supplier may use more UV stabilizer than the other. Your change to a cheaper material may cost you more than sticking with the old supplier.
Chris DeArmitt PhD FRSC CChem
www.phantomplastics.com
Consultant to the plastics industry
RE: HDPE Wicker
Also, a good way to improve tensile in such a case is to improve elongation as that allows more load sharing between strands. An increase in molecular weight will improve both tensile and elongation and will also provide more in reserve to resist UV degradation.
UV degrades the polymer. Fading of pigments can be from UV or visible light so your comment re UV and fading is a bit off the mark.
A grade of HDPE with no nucleating agent present would help tensile and elongation. Many things like some pigments for instance can act as nucleating agents.
A small amount of vinyl acetate in the HDPE alos greatly improves elongation and stress crack formation. While it decreases tensile on lab test mouldings, it generally increases tensile of an unevenly loaded fabric as is the case in your outdoor furniture. Once again the effective tensile is improved by improved load sharing due to improved elongation.
Regards
Pat
See FAQ731-376: Eng-Tips.com Forum Policies for tips on use of eng-tips by professional engineers &
http://eng-tips.com/market.cfm
for site rules
RE: HDPE Wicker
1.tensile peak - 147.66 Kg/Cm Sq
2.tensile break - 142.68 Kg/Cm Sq
3.elogation peak - 23.86%
4.elogation Break - 760.57%
Now we need atleast 230 Kg/Cm Sq of tensile strength and the elongation is fine.
RE: HDPE Wicker
You said you use UV opaque pigments. The most popular is TiO2 (titanium dioxide) but that can actually attack your plastic when the sunlight hits unless you buy the right grade.
TiO2 when exposed to UV generates free radicals that rip your plastic to pieces. To prevent that, TiO2 is coated to shield the plastic from it. Some grades are well coated, others not.
Chris DeArmitt PhD FRSC CChem
www.phantomplastics.com
Consultant to the plastics industry
RE: HDPE Wicker
RE: HDPE Wicker
If the new items fail then adding elastomer will increase the elongation to break but slightly reduce the yield strength. So, if the former is your problem then great, if the strength was the issue then the elastomer will harm your product.
It is most likely that the TiO2, other pigments or lack of proper UV stabilizer are the problem, not the new properties. We can't tell you for sure, you'll have to do tests to find out.
Chris DeArmitt PhD FRSC CChem
www.phantomplastics.com
Consultant to the plastics industry
RE: HDPE Wicker
While elastomer decreases the strength of a single test bar, it can increase the strength of a woven fabric that has uneven load on a number of strands as the most heavily loaded strand yeilds more and allows the other strands to take a bigger portion of the total load. This is especially evident with higher MW but also shows up with elastomer.
The modifier of choice for PE manufacturers last time I was in the loop was VA. With up to 5% VA they don't even declare it as EVA, they simply call it high stress crack resistant PE.
Regards
Pat
See FAQ731-376: Eng-Tips.com Forum Policies for tips on use of eng-tips by professional engineers &
http://eng-tips.com/market.cfm
for site rules
RE: HDPE Wicker
Chris DeArmitt PhD FRSC CChem
www.phantomplastics.com