INTELLIGENT WORK FORUMS
FOR ENGINEERING PROFESSIONALS

Log In

Come Join Us!

Are you an
Engineering professional?
Join Eng-Tips Forums!
  • Talk With Other Members
  • Be Notified Of Responses
    To Your Posts
  • Keyword Search
  • One-Click Access To Your
    Favorite Forums
  • Automated Signatures
    On Your Posts
  • Best Of All, It's Free!
  • Students Click Here

*Eng-Tips's functionality depends on members receiving e-mail. By joining you are opting in to receive e-mail.

Posting Guidelines

Promoting, selling, recruiting, coursework and thesis posting is forbidden.

Students Click Here

Jobs

Test specimen for preferential weld attack

Test specimen for preferential weld attack

Test specimen for preferential weld attack

(OP)
Hello all, I am seeking a metallurical lab / company in the Houston area who could assist me with the following.

I need to preferentially corrode a mock up A516-70 welded specimen in the weld zone to given depths. (Mechanical means not acceptable)The piece will be 0.75" thick and I would like to corrode areas of the weld to 10% 20% 30% 50% wall loss increments to qualify an advanced NDE Technique for a specific damage mechanism.

Suggestions greatly appreciated.

RE: Test specimen for preferential weld attack

The Southwest Research Institute www.swri.edu in San Antonio might be worth a try.

RE: Test specimen for preferential weld attack

This isn't so difficult.  You can mask the various zones for different times and expose the sample in HCl or similar acid to get the corrosion-type trenches you seem to need. The electroplating folks have good masking paints. etc.  You can start with the whole area masked except where you want the deepest ditch, then remove the masking where you want the next deepest ditch, etc.,  exposing the steel for different times and controlling the depths.  
Alternatively you could make some mechanical grooves of different depths and then expose the whole weld zone to acid to get the rough-etched surface you may be looking for.

My company has its main metallurgical lab in Austin if you are interested.

RE: Test specimen for preferential weld attack

(OP)
Thank you for the tips. I may have someone to do electrochemical machining(EDM). Had thought of masking and HCl, but havenet found a lab to do it. If the EDM falls through I'll get the Austin Contact.

Regards

Red Flag This Post

Please let us know here why this post is inappropriate. Reasons such as off-topic, duplicates, flames, illegal, vulgar, or students posting their homework.

Red Flag Submitted

Thank you for helping keep Eng-Tips Forums free from inappropriate posts.
The Eng-Tips staff will check this out and take appropriate action.

Reply To This Thread

Posting in the Eng-Tips forums is a member-only feature.

Click Here to join Eng-Tips and talk with other members!


Resources