INTELLIGENT WORK FORUMS
FOR ENGINEERING PROFESSIONALS

Log In

Come Join Us!

Are you an
Engineering professional?
Join Eng-Tips Forums!
  • Talk With Other Members
  • Be Notified Of Responses
    To Your Posts
  • Keyword Search
  • One-Click Access To Your
    Favorite Forums
  • Automated Signatures
    On Your Posts
  • Best Of All, It's Free!
  • Students Click Here

*Eng-Tips's functionality depends on members receiving e-mail. By joining you are opting in to receive e-mail.

Posting Guidelines

Promoting, selling, recruiting, coursework and thesis posting is forbidden.

Students Click Here

Jobs

Question about A992 Structural Steel

Question about A992 Structural Steel

Question about A992 Structural Steel

(OP)
I'm curious if anyone has any experience of what this materials low temperature toughness characteristics are like?  How will it perform at -20, 0, 32 °F?

RE: Question about A992 Structural Steel

We have had occasion to test some failed parts. In the K-Zone of the web, absorbed energy values as low as 5 ft-lbs were obtained at 60 F. 20 to approximately 50 ft-lb absorbed energy values were obtained in the web away from the K-Zone at 20 F.  

Red Flag This Post

Please let us know here why this post is inappropriate. Reasons such as off-topic, duplicates, flames, illegal, vulgar, or students posting their homework.

Red Flag Submitted

Thank you for helping keep Eng-Tips Forums free from inappropriate posts.
The Eng-Tips staff will check this out and take appropriate action.

Reply To This Thread

Posting in the Eng-Tips forums is a member-only feature.

Click Here to join Eng-Tips and talk with other members!


Resources