INTELLIGENT WORK FORUMS
FOR ENGINEERING PROFESSIONALS

Log In

Come Join Us!

Are you an
Engineering professional?
Join Eng-Tips Forums!
  • Talk With Other Members
  • Be Notified Of Responses
    To Your Posts
  • Keyword Search
  • One-Click Access To Your
    Favorite Forums
  • Automated Signatures
    On Your Posts
  • Best Of All, It's Free!
  • Students Click Here

*Eng-Tips's functionality depends on members receiving e-mail. By joining you are opting in to receive e-mail.

Posting Guidelines

Promoting, selling, recruiting, coursework and thesis posting is forbidden.

Students Click Here

Jobs

Polypropylene and Butyl Rubber?

Polypropylene and Butyl Rubber?

Polypropylene and Butyl Rubber?

(OP)
I have a subwoofer, Infinity Reference 1230w, and the Polypropylene cone has separated from the Butyl Rubber Surround.  Is there an inexpensive adhesive suitable for this bonding the two back together?  I really have no idea where to look for this kind of thing, and I really wouldn't trust anyone at a hardware store.  Thanks.

RE: Polypropylene and Butyl Rubber?

This is very easy to accomplish with the use of a polyolefin primer which will raise the surface energy of the polypropylene but only for a window of time---usually 20 minutes.

Red Flag This Post

Please let us know here why this post is inappropriate. Reasons such as off-topic, duplicates, flames, illegal, vulgar, or students posting their homework.

Red Flag Submitted

Thank you for helping keep Eng-Tips Forums free from inappropriate posts.
The Eng-Tips staff will check this out and take appropriate action.

Reply To This Thread

Posting in the Eng-Tips forums is a member-only feature.

Click Here to join Eng-Tips and talk with other members!


Resources