Welding Stainless to Steel
Welding Stainless to Steel
(OP)
I need to weld some 304 stainless to AR steel.
I plan to use ER70S-6 wire and 75/25 gas.
This will be a fillet weld and will not be a load bearing weld.
I have been told that this will crack and fail, What are your thoughts?
I plan to use ER70S-6 wire and 75/25 gas.
This will be a fillet weld and will not be a load bearing weld.
I have been told that this will crack and fail, What are your thoughts?





RE: Welding Stainless to Steel
You need to use either ER 309 or Inconel (Ni-base filler metal).
RE: Welding Stainless to Steel
Use 309.
= = = = = = = = = = = = = = = = = = = =
Still trying to help you stop corrosion.
formerly Trent Tube, now Plymouth Tube
eblessman@plymouth.com
or edstainless@earthlink.net
RE: Welding Stainless to Steel
RC
All that is necessary for the triumph of evil is that good men do nothing.
Edmund Burke
RE: Welding Stainless to Steel
RE: Welding Stainless to Steel
Save water Drink Beer