Yield Strength For Superduplex
Yield Strength For Superduplex
(OP)
What is the yield strength value for superduplex SA 240- UNS No S32750 between temperature 50 Deg C and 350 Deg C. Please provide range temperature 50, 100, 150, 200, 250, 300, 350 Deg C.





RE: Yield Strength For Superduplex
Per ASME Section II, Part D, Table Y-1;
150 deg F 74 Ksi
200 deg F 70.5 Ksi
250 deg F 67.4 Ksi
300 64.7
400 60.7
500 58.3
600 57.2
650 57
to 750 57
Sorry, but you need to perform the conversions and interpolate accordingly.
The other source is from Outokumpu, their web site is provided below
http://
They list mechanical properties for SAF 2507 between 100 and 250 deg C.