cast aluminum mechanical properties
cast aluminum mechanical properties
(OP)
I'm looking for information regarding cast aluminum mechanical properties versus temperature for the temperature range of -40°C - + 70°C. Can anyone point me in the right direction? Specifically I'm looking for information for 356A and alloy 360.





RE: cast aluminum mechanical properties
OR ar-mmpds-01
RE: cast aluminum mechanical properties
RE: cast aluminum mechanical properties
http://www.matweb.com
That has a good deal of information on different materials.
Alan M. Etzkorn

Reliability Engineer
Wabash National Corp.
www.wabashnational.com
RE: cast aluminum mechanical properties
RE: cast aluminum mechanical properties
Depending on the geometry of your cast component, you may have to consider the possible occurance of porosity, it'll seriously deteriote the mechanical property.
Best regards,
ct
RE: cast aluminum mechanical properties
For 360 die cast
UTS 48.5 ksi @ -112F; 47.5ksi@ -18F;44 ksi @ +212F
TYS 27ksi @-112F; 28ksi@ -18F; 25ksi@ +212F
%E 4 @ -112F; 4 @ -18F; 2@ +212F
For 356-T7, sand cast
UTS 35 ksi @ -112F; 33ksi @ -18F; 30ksi @+ 212F
TYS 28.5ksi @ -112F; 27.5ksi @ -18F; 28ksi @ +212F
%E 3 @ -112F; 3 @ -18F; 2 @ +212F
These are all typical values, not guaranteed minimums.