B-H curve for 1018 steel
B-H curve for 1018 steel
(OP)
I am attempting to perform several magnetic analyses, but I couldn't find B-H curve for 1018 steel. I have read a former thread posted on 23-Jul-04, but I couldn't find any data with the link mentioned.
Could anyone send me these data? Thank you in advance.
Could anyone send me these data? Thank you in advance.





RE: B-H curve for 1018 steel
The following was taken from an FEA magnetic program for 1018 low carbon alloy. It also contains data for highly saturated condition.
B (Tesla) H (amp/m)
0.250300 238.73
0.925000 795.78
1.250000 1591.55
1.390000 2387.33
1.525000 3978.88
1.710000 7957.75
1.870000 15915.50
1.955000 23873.25
2.020000 39788.75
2.110000 79577.50
2.225000 159155.00
2.430000 318310.00
RE: B-H curve for 1018 steel
RE: B-H curve for 1018 steel
RE: B-H curve for 1018 steel
It is better to start a new thread when one has a new/different question.
There is a list of some magnetic modeling software packages in the FAQ section: See FAQ340-1112