Copper Pipe - Strain Hardening?
Copper Pipe - Strain Hardening?
(OP)
I am going to try hydroforming a copper water pipe into a new shape. My question is, how much will standard copper water pipe strain harden when formed? I looked and in Canada the spec is ASTM B75-C12200. My info says that is 99.9% pure copper.
Does anyone have any ideas of the hardening of copper pipe? I am running some FEA to predict the pressure required for forming and it is very dependent on the hardenability of the pipe.
Thank You
Does anyone have any ideas of the hardening of copper pipe? I am running some FEA to predict the pressure required for forming and it is very dependent on the hardenability of the pipe.
Thank You





RE: Copper Pipe - Strain Hardening?
RE: Copper Pipe - Strain Hardening?
RE: Copper Pipe - Strain Hardening?
UTS (Ksi)
30 @ 0% CW
40 @ 10%
50 @ 30%
53 @ 50%
58 @ >60%
YS (Ksi)
25 @ 0% CW
30 @ 10%
40 @ 30%
49 @ 50%
52 @ >60%
RE: Copper Pipe - Strain Hardening?
Thanks to all for the information provided.
RE: Copper Pipe - Strain Hardening?
Percent cold work is expressed as a percentage of strain deformation.