(OP)
Hello,
I'm looking for the right calculation method for calculating the length of the neutral line of a piece of sheet metal after bending it into a tube.
We use 304 and 316L stainless steel. I know it depents on a lot of properties (type, temp, etc). I'm looking for a methode that is as accurate as possible.
Thanks a lot...
I'm looking for the right calculation method for calculating the length of the neutral line of a piece of sheet metal after bending it into a tube.
We use 304 and 316L stainless steel. I know it depents on a lot of properties (type, temp, etc). I'm looking for a methode that is as accurate as possible.
Thanks a lot...





RE: Length of neutral line after bending sheet metal
Garland E. Borowski, PE
RE: Length of neutral line after bending sheet metal
R<2T X=0.33T
R=2T to 4T X=0.4T
R>4T X=0.5T
Best regards,
ct
RE: Length of neutral line after bending sheet metal
The location of the line must of course change - limct's post provides a good approximation of how much.
RE: Length of neutral line after bending sheet metal