B-H-curves
B-H-curves
(OP)
I'm looking for a B-H-curve of the stainless steel 1.4104 (AISI 430 F). Does anyone know where I can find it on the internet?
INTELLIGENT WORK FORUMS
FOR ENGINEERING PROFESSIONALS Come Join Us!Are you an
Engineering professional? Join Eng-Tips Forums!
*Eng-Tips's functionality depends on members receiving e-mail. By joining you are opting in to receive e-mail. Posting GuidelinesJobs |
|
RE: B-H-curves
However, this will give the flux density up to magnetizing force of 100 Orsteds.
You may need to go through the registration process to reach this page.
A better B-H graph you should find in ASM metals handbooks which will give the flux density up to very high magnetizing force (saturaion).
RE: B-H-curves
ANNEALED (75.5 HRB)
1450F 2 hours dry H2
H (Oe) B (Gauss)
0.00 0.00
0.39 85.05
0.92 340.21
1.45 595.36
1.71 850.52
2.11 1275.77
2.24 1615.98
2.37 2041.24
2.50 2466.49
2.63 2891.75
2.89 3487.11
3.03 4167.53
3.16 4762.89
3.29 5188.14
3.42 5783.51
3.55 6463.92
3.68 7144.33
3.95 7824.74
4.21 8420.10
4.47 8930.41
4.74 9355.67
5.00 9865.98
5.39 10376.30
5.79 10886.60
6.18 11226.80
7.11 11652.10
7.76 11907.20
9.08 12332.50
10.26 12502.60
11.45 12757.70
13.16 12927.80
14.74 13012.90
16.32 13183.00
17.89 13268.00
19.08 13353.10
22.24 13523.20
23.95 13608.20
25.39 13693.30
26.58 13693.30
27.89 13778.40
28.82 13778.40
29.87 13778.40
31.58 13706.30
39.47 13881.00
46.05 14055.60
57.89 14317.50
69.74 14579.40
82.89 14841.30
97.37 15015.90
114.47 15277.80
128.95 15452.40
142.11 15539.70
157.90 15714.30
175.00 15888.90
190.79 15976.20
206.58 16063.50
227.63 16150.80
246.05 16238.10
264.47 16325.40
282.90 16412.70
300.00 16412.70
RE: B-H-curves
= = = = = = = = = = = = = = = = = = = =